steel pipe
Magnetic Particle Inspection Of Forged Steel Parts
1) Characteristics of flaw detection of forged steel parts: forging processing forming methods are generally divided into two categories: free forging and die forging.
Its technological process is: blanking, heating, forging, (trimming) - detection, mechanical processing, heat treatment, inspection - (surface heat treatment, inspection) - surface treatment, finished product delivery.
In the forging process, cracks, folds and white spots are easy to occur. Heat treatment will produce quenching crack; Machining will produce grinding cracks and correction cracks; Surface heat treatment also produces cracks.
(2) Selection of flaw detection method: The fixed magnetic particle flaw detection machine is generally used for circumferential and longitudinal magnetization. If the remanence and coercivity of the material meet the requirements, remanence flaw detection method is recommended.
(3) Magnetic particle inspection of crankshaft
Inspection method: direct electrification circumferential magnetization, check forging cracks, folding, grinding cracks, quenching cracks, and hair lines, etc. Longitudinal magnetization of segmented coil, check transverse cracks including forging cracks, grinding cracks, correction cracks, quenching cracks and so on. Special attention should be paid to the observation of the corner and the edge of the oil injection hole.
Magnetic particle inspection of steel castings
(1) Characteristics of magnetic particle flaw detection of steel castings: steel castings are generally complicated in shape, and the types and positions of defects are relatively regular. The main defects are casting crack, loose, shrinkage cavity, inclusion, air hole and cold insulation, etc.
(2) Selection of flaw detection method: casting is generally small in volume, which is convenient for flaw detection on fixed flaw detection machine. All castings shall be tested for circumferential and longitudinal magnetization. The continuous method is used for flaw detection before heat treatment, and the remanence method is generally used for flaw detection after heat treatment. Dc flaw detection should be used to check air holes and inclusions under the surface. Fluorescent magnetic particle inspection is the best method for reticular cracks.
(3) CAM magnetic particle inspection
Testing method: continuous testing method is used for wool embryo, remanence testing method is used after heat treatment. The wheel part was tested by rod piercing method, and the shaft part was circumferentially magnetized by direct electrification method, and then magnetized longitudinally by coil. Focus on inspecting the cracks in the root position.
Magnetic particle inspection of special equipment in service and maintenance parts
(1) Features of magnetic particle inspection in service and maintenance parts: fatigue cracks and stress corrosion cracks are mainly found. The crack location is directly related to the stress condition. In the service and maintenance parts of the inspection conditions are poor, and the fatigue crack is small, as far as possible under the condition of the permit fluorescent magnetic particle inspection. Bolt holes should be threaded rod method, and use endoscope and other techniques. Small bolt holes can also be tested by rubber casting method.
(2) Magnetic particle inspection of bolts: bolts are fasteners and are subject to tensile force, which is easy to produce transverse fatigue cracks. Therefore, longitudinal magnetization of coils should be adopted. Remanence method and fluorescent magnetic particle inspection with lower concentration has the best effect.
Magnetic particle inspection of special workpiece:
(1) compression spring flaw detection: first, directly energized, check the longitudinal defects on the steel wire; Then the transverse defects on the steel wire are inspected by rod penetration method. Note: The spring should be rotated continuously during demagnetization.
(2) tensile spring flaw detection: first pull the spring (when necessary with tension machine) and an insulating rod to support, so that the springs each circle away from each other, and then directly energized, check the longitudinal defects on the wire. Then in each ring of the spring pad insulation (remove the support rod), with the rod through the method of flaw detection, check the transverse defects on the wire.